Rubber has good resistance to mild acids and alkalis, salts, and chlorine solutions. It has poor resistance to oils and solvents and is not recommended for use with ozone. Its temperature range is very limited.
Rubber with textile inserts suitable for current applications, without specific heat-resistance characteristics. Good resistance to ozone and atmospheric agents. It is usually cut and used for industrial lining. It is the most popularly used rubber on the market.
Sr. No. | Compounds | Natural Rubber | Neoprene | Nitrile (100% Pure) | EPDM (100% Pure) | Silicone | Viton | |
Properties | Unit | |||||||
1 | Hardness | Shore A | 55±5 | 70±5 | 60±5 | 60±5 | 65±5 | 72±5 |
2 | Tensile Strength (min) | Kg/cm2 | 50 | 50 | 100 | 80 | 50 | 40 |
3 | Elongation at Break (min) | % | 250 | 250 | 350 | 250 | 250 | 200 |
4 | Compression Set (70°C/24hrs/25% compression) | % | 50 | 45 | 30 | 50 | 45 | 55 |
5 | Volume Swell | |||||||
In IRM Oil No. 1 | % | NR | +27% | -2% | NR | -1% | -6% | |
In IRM Oil No. 2 | % | NR | +39% | +4% | NR | +7% | -1% | |
In IRM Oil No. 3 | % | NR | +75% | +15% | NR | +17% | +5% | |
6 | Chemical Resistance | |||||||
Dilute Acids & Bases | GOOD | FAIR | GOOD | GOOD | EXCELLENT | EXCELLENT | ||
Conc. Acids | FAIR | Not Recommended | Not Recommended | Not Recommended | EXCELLENT | EXCELLENT | ||
Oils | Not Recommended | Not Recommended | EXCELLENT | Not Recommended | FAIR | VERY GOOD | ||
Solvents | Not Recommended | Not Recommended | GOOD | Not Recommended | FAIR | VERY GOOD | ||
7 | Temperature Range | °C | -30°C to 70°C | -25°C to 80°C | -25°C to 110°C | -30°C to 90°C | -50°C to 220°C | -50°C to 220°C |
8 | Colour | BLACK | BLACK | BLACK | BLACK | BRICK RED/WHITE | BLACK |